| Standard | Nearest ISO Designation | International Equivalence | Chemical Composition by Wt. % | Conditions | |||||
| Cu% | Sn% | P% | Pb% | Zn% | Others | ||||
| ASTM B-139 C54400 | CuSn4Pb4Zn4 | - | Rem | 3.5 - 4.5 | 0.01-0.50 max | 3.5-4.5 max | 1.5-4.5 | Fe-0.1 Total Imp 0.50% max | H |
| ASTM B505 C 83600 | CuSn5Pb5Zn5 | DIN 1705 RG-5 ISO 1338 BS 1400 LG-2 IS 318 SAE J461 , SAE J 462 | 84-86 | 4-6 | 0.05 max | 4-6 | 4-6 | Fe-0.10 max Total Imp 0.50% max | Un wrought |
| ASTM B505 C 93200 | CuSn7Pb7Zn3 | DIN 1705 RG-7 ISO 1338 BS 1400 LG-2 IS 318 SAE J461 , SAE J 462 | 81-85 | 6-8 | 0.05 max | 5-7 | 3-5 | Fe-0.10 max Total Imp 0.50% max | Un wrought |
| Standard | Mechanical Properties | Applications | |||
| UTS N/mm2 | E% | Y.S. Rp 0.2 N/mm2 |
Hardness HB |
||
| ASTM B-139 C54400 | 345-447 | 10-15 min | - | - |
Hard and half hard leaded bronze used for friction
parts at average speed and pressure it is used as bearings, sockets,
slides, nuts etc. |
| ASTM B505 C 83600 | 225 min | 16 min | 90 min | 60 min | Leaded Bronze with excellent friction abilt is suitable for bearings, rings imersed, oiless bearings, chemical industries. |
| ASTM B505 C 93200 | 240 min | 15 min | 128 min | 65 min | This type of Leaded Bronze used when in corrosive abrasive conditions. Having good machinability, application to machine bearing, bush, bolts, nuts, circeplings, bushing and for ball point pen etc. |
| *Rods/Bars
for electrical purposes the conductivity/resistivity shall be as agreed. * The examples above mentioned are only indicative. |
|||||